CoolPoly D series of thermally conductive plastics transfers heat, a characteristic previously unavailable in injection molding grade polymers. CoolPoly is lightweight, netshape moldable and allows design freedom in applications previously restricted to metals. The D series is electrically non-conductive and can be used for its dielectric properties.&&

Product Description
SupplierCelanese
GenericPPS
Material StatusCommercial: Active
FeaturesExcellent Processability,Thermal conductivity,Insulation,V-0
AvailabilitysNorth America,Latin America,Asia Pacific,Europe
Process MethodsInjection Molding

Technical Data
PHYSICALNominal valueUnitTest method
Density1.82g/cm³ISO 1183
Shrinkage rateASTM D955
MD0.20%
TD0.40%

MECHANICALNominal valueUnitTest method
Tensile modulus23600MPaISO 527-2
tensile strength
yield37.0MPaISO 527-2
Nominal tensile fracture strain0.16%ISO 527-2
Bending modulus19400MPaISO 178
bending strength69.0MPaISO 178

IMPACTNominal valueUnitTest method
Charpy Notched Impact Strength1.1kJ/m²ISO 179
Charpy Unnotch Impact strength2.5kJ/m²ISO 179

THERMALNominal valueUnitTest method
Hot deformation temperature
0.45 MPa, unannealed276ISO 75-2/B
1.8 MPa, unannealed239ISO 75-2/A
Linear coefficient of thermal expansionISO 11359-2
MD6.5E-61/℃
TD5.0E-61/℃
Thermal conductivity coefficient10W/m/KASTM C177

Electrical performanceNominal valueUnitTest method
Surface resistivity4.5E+14ohmsASTM D257
Volume resistivity2.5E+16ohms·cmASTM D257
Dielectric strength29kV/mmASTM D149
Dielectric constantASTM D150
100 Hz4.80
1 MHz3.70
Dissipation factorASTM D150
100 Hz0.022
1 MHz2.3E-3
Arc resistance300secASTM D495
Compared to the leakage tracing index580VUL 746
Hot wire ignition
HWI120secUL 746

FLAME CHARACTERISTICSNominal valueUnitTest method
1.00 mmV-0UL 94

Process Conditions
injectionNominal valueUnitTest method
Drying temperature150°C
Drying time6.0hr
Dew Point-40.0°C
Recommended maximum moisture content0.0%
Barrel rear temperature290 to 315°C
Barrel middle temperature300 to 320°C
Barrel front temperature310 to 340°C
Nozzle temperature316 to 340°C
Processing (melt) temperature307 to 338°C
Mold temperature135 to 177°C
Injection pressure60.0 to 165MPa

Notes
【 Disclaimer 】
Guangzhou Soliao Information Technology Co., Ltd. reserves all rights. The information in this data table was obtained from the manufacturer of the material on soliao.com. Soliao.com makes every effort to ensure the accuracy of this data. However, the search company does not assume any responsibility for the uncertainty and consequences caused to users by these data values and suggestions, and strongly recommends verifying the data values with the material supplier before the final selection of materials.