Chemlon® 60GS6

About
60GS6 is a 30% glass sphere filled nylon 6.&&

Product Description
SupplierTeknor Apex
GenericPA6
Material StatusCommercial: Active
FeaturesHB
AvailabilitysEurope,North America
Process MethodsInjection Molding

Technical Data
PHYSICALNominal valueUnitTest method
Density1.35g/cm³ISO 1183
Molding shrinkage0.6-1.5%Internal Method
Water Absorption
Equilibrium, 23 ℃, 50% r. h2.0%ISO 62

MECHANICALNominal valueUnitTest method
Tensile Modulus
Dry3505.2MPaISO 527
Wet Cond1704.3MPaISO 527
Tensile Strength
Broken BRK, dry dry80.04MPaISO 527-2
Broken BRK, wet Cond40.02MPaISO 527-2
Tensile Strain
Broken BRK, dry dry10%ISO 527
Broken BRK, wet Cond20-50%ISO 527
Flexural Modulus
Dry2504.7MPaISO 178
Wet Cond1000.5MPaISO 178
Flexural Strength
Dry124.89MPaISO 178
Wet Cond60.03MPaISO 178

IMPACTNominal valueUnitTest method
Charpy Notched Impact Strength
Dry6.51kJ/m²ISO 179
Wet Cond11.97kJ/m²ISO 179
Charpy Unnotch Impact strength37.8kJ/m²ISO 179
Izod Notched Impact strength3.99KJ/m²ISO 180/1A

THERMALNominal valueUnitTest method
Hot deformation temperature HDT
0.45 MPa, dry205ISO 75-1/-2
0.45 MPa, wet cond185ISO 75-1/-2
1.82 MPa, dry70ISO 75-1/-2
1.82 MPa, wet cond65ISO 75-1/-2

ELECTRICALNominal valueUnitTest method
Surface Resistivity
Dry1E14ohmsIEC 60093
Wet Cond1E11ohmsIEC 60093
Volume Resistance
Dry1E16ohms·cmIEC 60093
Wet Cond1E14ohms·cmIEC 60093
Electric strength
Dry280V/milIEC 60243-1
Wet Cond200V/milIEC 60243-1
Relative permittivity
Dry3.8IEC 60250
Wet Cond4.2IEC 60250
Compared Tracking Index
Dry600VIEC 60112
Wet Cond500VIEC 60112

FLAME CHARACTERISTICSNominal valueUnitTest method
Flame Class Rating
0.8 mmHBUL 94
Oxygen Index24%ISO 4589-2

Process Conditions
Injection MoldingNominal valueUnitTest method
Drying Temperature80
Drying Time2.0hr
Rear Temperature Zone 1230-280
Middle Temperature Zone 2230-280
Front Temperature Zone 3230-280
Melt Temperature<300
Mold Temperature60-80
Injection Rate快速
Screw Speed50-200rpm

Notes
1. Typical properties: these are not to be construed as specifications.
2. Mould shrinkage is significantly influenced by many factors including wall thickness, gating, moulding shape and processing conditions. The range values given are determined from specimen bar mouldings of 1.5mm to 4mm wall thickness. They are provided as a guide for comparison purposes only and no guarantee should be inferred from their inclusion. (Specimens measured in the dry state, 24 hours after moulding).
3. Yield
4. Break
【 Disclaimer 】
Guangzhou Soliao Information Technology Co., Ltd. reserves all rights. The information in this data table was obtained from the manufacturer of the material on soliao.com. Soliao.com makes every effort to ensure the accuracy of this data. However, the search company does not assume any responsibility for the uncertainty and consequences caused to users by these data values and suggestions, and strongly recommends verifying the data values with the material supplier before the final selection of materials.