Texin® 950 U

About
Texin 950U resin is a polyether-based thermoplastic polyurethane with a Shore hardness of approximately 50D. It can be processed by injection molding or extrusion.&&

Product Description
SupplierCovestro
GenericTPU-醚
Material StatusCommercial: Active
FeaturesGood flexibility,High impact resistance,Hydrolysis stability,Good wear resistance,Heat Stabilized,High ESCR,Resistance to salt water/fog
AvailabilitysNorth America
Process MethodsExtrusion

Technical Data
PHYSICALNominal valueUnitTest method
Density1.15g/cm³ASTM D792
Density1.15g/cm³ISO 1183
Shrinkage rate ISO 2577
TD:2.54 mm0.80%ASTM D955
MD:2.54 mm0.80%ASTM D955
TD:2.54 mm0.80%ISO 2577
MD:2.54 mm0.80%ISO 2577

MECHANICALNominal valueUnitTest method
Shore hardness
Shaw’s D50 ISO 868
Shaw’s D50 ASTM D2240
Bending modulus ASTM D790
23℃114MPaASTM D790
70℃46.9MPaASTM D790
Bending modulus ISO 178
23℃114MPaISO 178
70℃46.9MPaISO 178
Taber abraser 
1000 cycles, 1000 g, H-18 wheels75.0mgISO 4649
1000 cycles, 1000 g, H-18 wheels75.0mgASTM D1044

elastic bodyNominal valueUnitTest method
tensile strength 
yield49.0MPaISO 37
yield49.0MPaASTM D412
300% strain27.6MPaISO 37
300% strain27.6MPaASTM D412
100% strain13.8MPaASTM D412
100% strain13.8MPaISO 37
50% strain12.1MPaISO 37
50% strain12.1MPaASTM D412
Tensile strain
fracture470%ASTM D412
fracture470%ISO 37
tear strength131kN/mASTM D624
tear strength130kN/mISO 34-1
Compression deformation ASTM D395B
23℃,22 hr15%ASTM D395B
23℃,22 hr20%ASTM D395B
70℃,22 hr40%ASTM D395B
70℃,22 hr70%ASTM D395B
Compression deformation ISO 815
23℃,22 hr20%ISO 815
23℃,22 hr15%ISO 815
70℃,22 hr70%ISO 815
70℃,22 hr40%ISO 815
Basho’s elasticity35%ASTM D2632

THERMALNominal valueUnitTest method
Embrittlement temperature< -68.0ASTM D746
Embrittlement temperature< -68.0ISO 974
Glass transition temperature-27.0DMA
Vicat Softening Temp128ASTM D1525 4
Vicat Softening Temp128ISO 306/50
Linear coefficient of thermal expansion
MD1.3E-41/℃ASTM D696

Aging performanceNominal valueUnitTest method
The rate of change in tensile strength in air ASTM D573
100℃,70 hr2.0%ASTM D573
100% Strain,100℃,70 hr4.0%ASTM D573
300% Strain,100℃,70 hr2.0%ASTM D573
100℃,168 hr2.0%ASTM D573
100% Strain,100℃,168 hr4.0%ASTM D573
300% Strain,100℃,168 hr-1.0%ASTM D573
100℃,336 hr4.0%ASTM D573
100% Strain,100℃,336 hr4.0%ASTM D573
300% Strain,100℃,336 hr-2.0%ASTM D573
100℃,504 hr38%ASTM D573
100% Strain,100℃,504 hr5.0%ASTM D573
300% Strain,100℃,504 hr-3.0%ASTM D573
125℃,70 hr-11%ASTM D573
100% Strain,125℃,70 hr1.0%ASTM D573
300% Strain,125℃,70 hr-7.0%ASTM D573
125℃,168 hr-27%ASTM D573
100% Strain,125℃,168 hr4.0%ASTM D573
300% Strain,125℃,168 hr-18%ASTM D573
125℃,336 hr-40%ASTM D573
100% Strain,125℃,336 hr0.0%ASTM D573
300% Strain,125℃,336 hr-22%ASTM D573
125℃,504 hr-44%ASTM D573
100% Strain,125℃,504 hr-5.0%ASTM D573
300% Strain,125℃,504 hr-25%ASTM D573
The rate of change in tensile strength in air ISO 216
100℃,70 hr2.0%ISO 216
100% Strain 100℃,70 hr4.0%ISO 216
300% Strain 100℃,70 hr2.0%ISO 216
100℃,168 hr2.0%ISO 216
100% Strain 100℃,168 hr4.0%ISO 216
300% Strain 100℃,168 hr-1.0%ISO 216
100℃,336 hr4.0%ISO 216
100% Strain 100℃,336 hr4.0%ISO 216
300% Strain 100℃,336 hr-2.0%ISO 216
100℃,504 hr38%ISO 216
100% Strain 100℃,504 hr5.0%ISO 216
300% Strain 100℃,504 hr-3.0%ISO 216
125℃,70 hr-11%ISO 216
100% Strain 125℃,70 hr1.0%ISO 216
300% Strain 125℃,70 hr-7.0%ISO 216
125℃,168 hr-27%ISO 216
100% strain 125 ℃, 168 hr4.0%ISO 216
300% Strain 125℃,168 hr-18%ISO 216
125℃,336 hr-40%ISO 216
100% Strain 125℃,336 hr0.0%ISO 216
300% Strain 125℃,336 hr-22%ISO 216
125℃,504 hr-44%ISO 216
100% Strain 125℃,504 hr-5.0%ISO 216
300% Strain 125℃,504 hr-25%ISO 216
The rate of change in ultimate elongation in air ASTM D573
100℃,70 hr10%ASTM D573
100℃,168 hr15%ASTM D573
100℃,336 hr19%ASTM D573
100℃,504 hr16%ASTM D573
125℃,70 hr22%ASTM D573
125℃,168 hr29%ASTM D573
125℃,336 hr12%ASTM D573
125℃,504 hr9.0%ASTM D573
Changes in tensile stress during fracture in air ISO 216
100℃,70 hr10%ISO 216
100℃,168 hr15%ISO 216
100℃,336 hr19%ISO 216
100℃,504 hr16%ISO 216
125℃,70 hr22%ISO 216
125℃,168 hr29%ISO 216
125℃,336 hr12%ISO 216
125℃,504 hr9.0%ISO 216
The rate of change in hardness of a hardness tester in the air ASTM D573
Shore D, 100 ℃, 70 hr-1.0 ASTM D573
Shore D, 100 ℃, 168 hr0.0 ASTM D573
Shore D, 100 ℃, 336 hr-2.0 ASTM D573
Shore D, 100 ℃, 504 hr-1.0 ASTM D573
Shore D, 125 ℃, 70 hr1.0 ASTM D573
Support D, 125 ℃, 168 hr-1.0 ASTM D573
Shaw’s D, 125 ℃, 336 hr-1.0 ASTM D573
Shaw’s D, 125 ℃, 504 hr1.0 ASTM D573
The rate of change of Shore hardness in air ISO 216
Shore D, 100 ℃, 70 hr-1.0 ISO 216
Shore D, 100 ℃, 168 hr0.0 ISO 216
Shore D, 100 ℃, 336 hr-2.0 ISO 216
Shore D, 100 ℃, 504 hr-1.0 ISO 216
Shore D, 125 ℃, 70 hr1.0 ISO 216
Support D, 125 ℃, 168 hr-1.0 ISO 216
Shaw’s D, 125 ℃, 336 hr-1.0 ISO 216
Shaw’s D, 125 ℃, 504 hr1.0 ISO 216
The rate of change in tensile strength ASTM D471
23℃,70 hr,in Reference Fuel A(Isooctane)16%ASTM D471
100% Strain,23℃,70 hr,in Reference Fuel A(Isooctane)-3.0%ASTM D471
300% Strain,23℃,70 hr,in Reference Fuel A(Isooctane)0.0%ASTM D471
23 ℃, 70 hr, methanol-17%ASTM D471
100% Strain,23℃,70 hr,in Reference Fuel C-42%ASTM D471
300% Strain,23℃,70 hr,in Reference Fuel C-36%ASTM D471
23℃,168 hr,in Reference Fuel A(Isooctane)16%ASTM D471
100% Strain,23℃,168 hr,in Reference Fuel A(Isooctane)6.0%ASTM D471
300% Strain,23℃,168 hr,in Reference Fuel A(Isooctane)2.0%ASTM D471
23 ℃, 168 hr, methanol-17%ASTM D471
100% Strain,23℃,168 hr,in Reference Fuel C-36%ASTM D471
300% Strain,23℃,168 hr,in Reference Fuel C-30%ASTM D471
23℃,336 hr,in Reference Fuel A(Isooctane)7.0%ASTM D471
100% Strain,23℃,336 hr,in Reference Fuel A(Isooctane)1.0%ASTM D471
300% Strain,23℃,336 hr,in Reference Fuel A(Isooctane)3.0%ASTM D471
23℃,336 hr,in Reference Fuel C-20%ASTM D471
100% Strain,23℃,336 hr,in Reference Fuel C-36%ASTM D471
300% Strain,23℃,336 hr,in Reference Fuel C-33%ASTM D471
23℃,504 hr,in Reference Fuel A(Isooctane)13%ASTM D471
100% Strain,23℃,504 hr,in Reference Fuel A(Isooctane)-4.0%ASTM D471
300% Strain,23℃,504 hr,in Reference Fuel A(Isooctane)-4.0%ASTM D471
23℃,504 hr,in Reference Fuel C-15%ASTM D471
100% Strain,23℃,504 hr,in Reference Fuel C-36%ASTM D471
300% Strain,23℃,504 hr,in Reference Fuel C-51%ASTM D471
100 ℃, 70 hr, in ASTM # 1 oil2.0%ASTM D471
100% Strain,100℃,70 hr,in ASTM #1 Oil7.0%ASTM D471
300% Strain,100℃,70 hr,in ASTM #1 Oil0.0%ASTM D471
100 ℃, 70 hr, in ASTM # 3 oil10%ASTM D471
100% Strain,100℃,70 hr,in ASTM #3 Oil2.0%ASTM D471
300% Strain,100℃,70 hr,in ASTM #3 Oil3.0%ASTM D471
100℃,168 hr,in ASTM #1 Oil0.0%ASTM D471
100% Strain,100℃,168 hr,in ASTM #1 Oil4.0%ASTM D471
300% Strain,100℃,168 hr,in ASTM #1 Oil0.0%ASTM D471
100℃,168 hr,in ASTM #3 Oil12%ASTM D471
100% Strain,100℃,168 hr,in ASTM #3 Oil-7.0%ASTM D471
300% Strain,100℃,168 hr,in ASTM #3 Oil-11%ASTM D471
100℃,336 hr,in ASTM #1 Oil-2.0%ASTM D471
100% Strain,100℃,336 hr,in ASTM #1 Oil8.0%ASTM D471
300% Strain,100℃,336 hr,in ASTM #1 Oil0.0%ASTM D471
100℃,336 hr,in ASTM #3 Oil-3.0%ASTM D471
100% Strain,100℃,336 hr,in ASTM #3 Oil-2.0%ASTM D471
300% Strain,100℃,336 hr,in ASTM #3 Oil-9.0%ASTM D471
100℃,504 hr,in ASTM #1 Oil-3.0%ASTM D471
100% Strain,100℃,504 hr,in ASTM #1 Oil4.0%ASTM D471
300% Strain,100℃,504 hr,in ASTM #1 Oil-7.0%ASTM D471
100℃,504 hr,in ASTM #3 Oil1.0%ASTM D471
100% Strain,100℃,504 hr,in ASTM #3 Oil-9.0%ASTM D471
300% Strain,100℃,504 hr,in ASTM #3 Oil-18%ASTM D471
The rate of change in tensile strength ISO 175
23℃,70 hr,in Reference Fuel A(Isooctane)16%ISO 175
100% Strain,23℃,70 hr,in Reference Fuel A(Isooctane)-3.0%ISO 175
300% Strain,23℃,70 hr,in Reference Fuel A(Isooctane)0.0%ISO 175
23 ℃, 70 hr, methanol-17%ISO 175
100% Strain,23℃,70 hr,in Reference Fuel C-42%ISO 175
300% Strain,23℃,70 hr,in Reference Fuel C-36%ISO 175
23℃,168 hr,in Reference Fuel A(Isooctane)16%ISO 175
100% Strain,23℃,168 hr,in Reference Fuel A(Isooctane)6.0%ISO 175
300% Strain,23℃,168 hr,in Reference Fuel A(Isooctane)2.0%ISO 175
23 ℃, 168 hr, methanol-17%ISO 175
100% Strain,23℃,168 hr,in Reference Fuel C-36%ISO 175
300% Strain,23℃,168 hr,in Reference Fuel C-30%ISO 175
23℃,336 hr,in Reference Fuel A(Isooctane)7.0%ISO 175
100% Strain,23℃,336 hr,in Reference Fuel A(Isooctane)1.0%ISO 175
300% Strain,23℃,336 hr,in Reference Fuel A(Isooctane)3.0%ISO 175
23℃,336 hr,in Reference Fuel C-20%ISO 175
100% Strain,23℃,336 hr,in Reference Fuel C-36%ISO 175
300% Strain,23℃,336 hr,in Reference Fuel C-33%ISO 175
23℃,504 hr,in Reference Fuel A(Isooctane)13%ISO 175
100% Strain,23℃,504 hr,in Reference Fuel A(Isooctane)-4.0%ISO 175
300% Strain,23℃,504 hr,in Reference Fuel A(Isooctane)-4.0%ISO 175
23℃,504 hr,in Reference Fuel C-15%ISO 175
100% Strain,23℃,504 hr,in Reference Fuel C-36%ISO 175
300% Strain,23℃,504 hr,in Reference Fuel C-51%ISO 175
100 ℃, 70 hr, in ASTM # 1 oil2.0%ISO 175
100% Strain,100℃,70 hr,in ASTM #1 Oil7.0%ISO 175
300% Strain,100℃,70 hr,in ASTM #1 Oil0.0%ISO 175
100 ℃, 70 hr, in ASTM # 3 oil10%ISO 175
100% Strain,100℃,70 hr,in ASTM #3 Oil2.0%ISO 175
300% Strain,100℃,70 hr,in ASTM #3 Oil3.0%ISO 175
100℃,168 hr,in ASTM #1 Oil0.0%ISO 175
100% Strain,100℃,168 hr,in ASTM #1 Oil4.0%ISO 175
300% Strain,100℃,168 hr,in ASTM #1 Oil0.0%ISO 175
100℃,168 hr,in ASTM #3 Oil12%ISO 175
100% Strain,100℃,168 hr,in ASTM #3 Oil-7.0%ISO 175
300% Strain,100℃,168 hr,in ASTM #3 Oil-11%ISO 175
100℃,336 hr,in ASTM #1 Oil-2.0%ISO 175
100% Strain,100℃,336 hr,in ASTM #1 Oil8.0%ISO 175
300% Strain,100℃,336 hr,in ASTM #1 Oil0.0%ISO 175
100℃,336 hr,in ASTM #3 Oil-3.0%ISO 175
100% Strain,100℃,336 hr,in ASTM #3 Oil-2.0%ISO 175
300% Strain,100℃,336 hr,in ASTM #3 Oil-9.0%ISO 175
100℃,504 hr,in ASTM #1 Oil-3.0%ISO 175
100% Strain,100℃,504 hr,in ASTM #1 Oil4.0%ISO 175
300% Strain,100℃,504 hr,in ASTM #1 Oil-7.0%ISO 175
100℃,504 hr,in ASTM #3 Oil1.0%ISO 175
100% Strain,100℃,504 hr,in ASTM #3 Oil-9.0%ISO 175
300% Strain,100℃,504 hr,in ASTM #3 Oil-18%ISO 175
Change rate of ultimate elongation ASTM D471
23℃,70 hr,in Reference Fuel A(Isooctane)5.0%ASTM D471
23 ℃, 70 hr, methanol0.0%ASTM D471
23℃,168 hr,in Reference Fuel A(Isooctane)7.0%ASTM D471
23 ℃, 168 hr, methanol-6.0%ASTM D471
23℃,336 hr,in Reference Fuel A(Isooctane)3.0%ASTM D471
23℃,336 hr,in Reference Fuel C-2.0%ASTM D471
23℃,504 hr,in Reference Fuel A(Isooctane)8.0%ASTM D471
23℃,504 hr,in Reference Fuel C-2.0%ASTM D471
100 ℃, 70 hr, in ASTM # 1 oil18%ASTM D471
100 ℃, 70 hr, in ASTM # 3 oil17%ASTM D471
100℃,168 hr,in ASTM #1 Oil19%ASTM D471
100℃,168 hr,in ASTM #3 Oil25%ASTM D471
100℃,336 hr,in ASTM #1 Oil23%ASTM D471
100℃,336 hr,in ASTM #3 Oil27%ASTM D471
100℃,504 hr,in ASTM #1 Oil32%ASTM D471
100℃,504 hr,in ASTM #3 Oil38%ASTM D471
Changes in tensile stress during fracture ISO 175
23℃,70 hr,in Reference Fuel A(Isooctane)5.0%ISO 175
23 ℃, 70 hr, methanol0.0%ISO 175
23℃,168 hr,in Reference Fuel A(Isooctane)7.0%ISO 175
23 ℃, 168 hr, methanol-6.0%ISO 175
23℃,336 hr,in Reference Fuel A(Isooctane)3.0%ISO 175
23℃,336 hr,in Reference Fuel C-2.0%ISO 175
23℃,504 hr,in Reference Fuel A(Isooctane)8.0%ISO 175
23℃,504 hr,in Reference Fuel C-2.0%ISO 175
100 ℃, 70 hr, in ASTM # 1 oil18%ISO 175
100 ℃, 70 hr, in ASTM # 3 oil17%ISO 175
100℃,168 hr,in ASTM #1 Oil19%ISO 175
100℃,168 hr,in ASTM #3 Oil25%ISO 175
100℃,336 hr,in ASTM #1 Oil23%ISO 175
100℃,336 hr,in ASTM #3 Oil27%ISO 175
100℃,504 hr,in ASTM #1 Oil32%ISO 175
100℃,504 hr,in ASTM #3 Oil38%ISO 175
The rate of change in Shore hardness ASTM D471
Shore D, 23 ℃, 70 hr, in reference fuel A (isooctane)1.0 ASTM D471
Shore D, 23°C, 70 hr, in Reference Fuel C-11 ASTM D471
Shore D, 23 ℃, 168 hr, in reference fuel A (isooctane)1.0 ASTM D471
Shore D, 23 ℃, 168 hr, in reference fuel-13 ASTM D471
Shore D, 23 ℃, 336 hr, in reference fuel A (isooctane)0.0 ASTM D471
Shore D, 23 ℃, 336 hr, in reference fuel C-10 ASTM D471
Shore D, 23 ℃, 504 hr, in reference fuel A (isooctane)2.0 ASTM D471
Shore D, 23 ℃, 504 hr, in reference fuel C-13 ASTM D471
Shore D, 100°C, 70 hr, in ASTM #1 Oil0.0 ASTM D471
Shore D, 100 ℃, 70 hr, in ASTM # 3 oil5.0 ASTM D471
Shore D, 100°C, 168 hr, in ASTM #1 Oil2.0 ASTM D471
Shore D, 100 ℃, 168 hr, in ASTM # 3 oil5.0 ASTM D471
Shore D, 100 ℃, 336 hr, in ASTM # 1 oil0.0 ASTM D471
Shore D, 100 ℃, 336 hr, in ASTM # 3 oil-4.0 ASTM D471
Shore D, 100 ℃, 504 hr, in ASTM # 1 oil2.0 ASTM D471
Shore D, 100 ℃, 504 hr, in ASTM # 3 oil-2.0 ASTM D471
The rate of change in Shore hardness ISO 175
Shore D, 23 ℃, 70 hr, in reference fuel A (isooctane)1.0 ISO 175
Shore D, 23°C, 70 hr, in Reference Fuel C-11 ISO 175
Shore D, 23 ℃, 168 hr, in reference fuel A (isooctane)1.0 ISO 175
Shore D, 23 ℃, 168 hr, in reference fuel-13 ISO 175
Shore D, 23 ℃, 336 hr, in reference fuel A (isooctane)0.0 ISO 175
Shore D, 23 ℃, 336 hr, in reference fuel C-10 ISO 175
Shore D, 23 ℃, 504 hr, in reference fuel A (isooctane)2.0 ISO 175
Shore D, 23 ℃, 504 hr, in reference fuel C-13 ISO 175
Shore D, 100°C, 70 hr, in ASTM #1 Oil0.0 ISO 175
Shore D, 100 ℃, 70 hr, in ASTM # 3 oil5.0 ISO 175
Shore D, 100°C, 168 hr, in ASTM #1 Oil2.0 ISO 175
Shore D, 100 ℃, 168 hr, in ASTM # 3 oil5.0 ISO 175
Shore D, 100 ℃, 336 hr, in ASTM # 1 oil0.0 ISO 175
Shore D, 100 ℃, 336 hr, in ASTM # 3 oil-4.0 ISO 175
Shore D, 100 ℃, 504 hr, in ASTM # 1 oil2.0 ISO 175
Shore D, 100 ℃, 504 hr, in ASTM # 3 oil-2.0 ISO 175
Volume change ASTM D471
23℃,70 hr,in Reference Fuel A0.0%ASTM D471
23 ℃, 70 hr, methanol22%ASTM D471
23℃,168 hr,in Reference Fuel A1.0%ASTM D471
23 ℃, 168 hr, methanol26%ASTM D471
23℃,336 hr,in Reference Fuel A1.0%ASTM D471
23℃,336 hr,in Reference Fuel C26%ASTM D471
23℃,504 hr,in Reference Fuel A1.0%ASTM D471
23℃,504 hr,in Reference Fuel C26%ASTM D471
100 ℃, 70 hr, in ASTM # 1 oil0.0%ASTM D471
100 ℃, 70 hr, in ASTM # 3 oil9.0%ASTM D471
100℃,168 hr,in ASTM #1 Oil0.0%ASTM D471
100℃,168 hr,in ASTM #3 Oil10%ASTM D471
100℃,336 hr,in ASTM #1 Oil0.0%ASTM D471
100℃,336 hr,in ASTM #3 Oil12%ASTM D471
100℃,504 hr,in ASTM #1 Oil0.0%ASTM D471
100℃,504 hr,in ASTM #3 Oil13%ASTM D471
Volume change ISO 175
23℃,70 hr,in Reference Fuel A0.0%ISO 175
23 ℃, 70 hr, methanol22%ISO 175
23℃,168 hr,in Reference Fuel A1.0%ISO 175
23 ℃, 168 hr, methanol26%ISO 175
23℃,336 hr,in Reference Fuel A1.0%ISO 175
23℃,336 hr,in Reference Fuel C26%ISO 175
23℃,504 hr,in Reference Fuel A1.0%ISO 175
23℃,504 hr,in Reference Fuel C26%ISO 175
100 ℃, 70 hr, in ASTM # 1 oil0.0%ISO 175
100 ℃, 70 hr, in ASTM # 3 oil9.0%ISO 175
100℃,168 hr,in ASTM #1 Oil0.0%ISO 175
100℃,168 hr,in ASTM #3 Oil10%ISO 175
100℃,336 hr,in ASTM #1 Oil0.0%ISO 175
100℃,336 hr,in ASTM #3 Oil12%ISO 175
100℃,504 hr,in ASTM #1 Oil0.0%ISO 175
100℃,504 hr,in ASTM #3 Oil13%ISO 175

Supplementary informationNominal valueUnitTest method
Compression load ASTM D575
10% deflection5.52MPaASTM D575
15% deflection7.58MPaASTM D575
2% deflection1.03MPaASTM D575
20% deflection10.3MPaASTM D575
25% deflection12.4MPaASTM D575
5% deflection2.93MPaASTM D575
50% deflection31.0MPaASTM D575

Process Conditions
injectionNominal valueUnitTest method
ExtrusionNominal valueUnitTest method
Drying temperature – hot air dryer99 to 110°C
Drying time – hot air dryer2.0hr
Recommended maximum moisture content< 0.030%
Recommended injection volume40 to 80%
Proposed maximum recycled material ratio20%
Barrel rear temperature180 to 200°C
Barrel middle temperature180 to 205°C
Barrel front temperature180 to 210°C
Nozzle temperature185 to 210°C
Processing (melt) temperature205°C
Mold temperature15 to 45°C
Injection pressure41.4 to 96.5MPa
Clamping force4.1 to 6.9kN/cm²
Screw length to diameter ratio20.0:1.0 
Screw compression ratio2.5:1.0 to 3.0:1.0 
Drying temperature99 to 110°C
Drying time2.0hr
Barrel 1 zone temperature180 to 210°C
Barrel 2 zone temperature180 to 210°C
Barrel 3 zone temperature180 to 205°C
Melt temperature185 to 210°C
Nozzle temperature180 to 200°C

Notes
1. Typical properties: these are not to be construed as specifications.
2. Die C
3. Post-cured 16 hr at 230°F
4. Rate A (50°C/h)
【 Disclaimer 】
Guangzhou Soliao Information Technology Co., Ltd. reserves all rights. The information in this data table was obtained from the manufacturer of the material on soliao.com. Soliao.com makes every effort to ensure the accuracy of this data. However, the search company does not assume any responsibility for the uncertainty and consequences caused to users by these data values and suggestions, and strongly recommends verifying the data values with the material supplier before the final selection of materials.