About |
---|
Texin 250 resin is an aromatic polyester-based thermoplastic polyurethane with a Shore hardness of approximately 50D. It is processed primarily by extrusion and blow molding but can also be used for injection molding.&& |
Product Description | |
---|---|
Supplier | Covestro |
Generic | TPU-酯 |
Material Status | Commercial: Active |
Features | Low speed solidification point,Good wear resistance,Grease resistance,Solvent resistance |
Availabilitys | North America |
Technical Data | |||
---|---|---|---|
PHYSICAL | Nominal value | Unit | Test method |
Density | 1.22 | g/cm³ | ASTM D792 , ISO 1183 |
Shrinkage rate | |||
MD:2.54 mm | 0.80 | % | ASTM D955 |
TD:2.54 mm | 0.80 | % | ASTM D955 |
TD:2.54 mm | 0.80 | % | ISO 2577 |
MD:2.54 mm | 0.80 | % | ISO 2577 |
elastic body | Nominal value | Unit | Test method |
---|---|---|---|
tensile strength | ASTM D412 , ISO 37 | ||
yield | 46.2 | MPa | ASTM D412 , ISO 37 |
100% strain | 11.7 | MPa | ASTM D412 , ISO 37 |
300% strain | 31.7 | MPa | ASTM D412 , ISO 37 |
Tensile strain | |||
fracture | 400 | % | ASTM D412,ISO 37 |
tear strength | |||
— | 136 | kN/m | ASTM D624 |
— | 140 | kN/m | ISO 34-1 |
Compression deformation | ASTM D395B , ISO 815 | ||
23℃,22 hr | 15 | % | ASTM D395B,ISO 815 |
70℃,22 hr | 35 | % | ASTM D395B,ISO 815 |
Basho’s elasticity | 25 | % | ASTM D2632 |
THERMAL | Nominal value | Unit | Test method |
---|---|---|---|
Glass transition temperature | -20.0 | ℃ | DMA |
Vicat Softening Temp | |||
A50 | 115 | ℃ | ASTM D1525,ISO 306 |
MECHANICAL | Nominal value | Unit | Test method |
---|---|---|---|
Shore hardness | ASTM D2240 , ISO 868 | ||
Shaw’s A | 95 | ASTM D2240 , ISO 868 | |
Shaw’s D | 50 | ASTM D2240 , ISO 868 | |
Bending modulus | ASTM D790 , ISO 178 | ||
23℃ | 83.0 | MPa | ASTM D790 , ISO 178 |
70℃ | 36.0 | MPa | ASTM D790 , ISO 178 |
Taber abraser | |||
1000 cycles, 1000 g, H-18 wheels | 70.0 | mg | ASTM D1044 |
1000 cycles, 1000 g, H-18 wheels | 70.0 | mg | ISO 4649 |
Process Conditions | |||
---|---|---|---|
injection | Nominal value | Unit | Test method |
Extrusion | Nominal value | Unit | Test method |
Drying temperature – hot air dryer | 93 to 104 | °C | |
Drying time – hot air dryer | 2.0 | hr | |
Recommended maximum moisture content | 0.030 | % | |
Proposed maximum recycled material ratio | 20 | % | |
Barrel rear temperature | 190 to 210 | °C | |
Barrel middle temperature | 190 to 215 | °C | |
Barrel front temperature | 200 to 220 | °C | |
Nozzle temperature | 205 to 225 | °C | |
Processing (melt) temperature | 205 to 215 | °C | |
Mold temperature | 15 to 40 | °C | |
Injection pressure | 41.4 to 103 | MPa | |
Injection speed | 慢to中等 | ||
Back pressure | < 1.38 | MPa | |
Screw speed | 40 to 80 | rpm | |
Cushion | 3.18 | mm | |
Drying temperature | 93 to 104 | °C | |
Drying time | 2.0 | hr | |
Barrel 1 zone temperature | 180 to 200 | °C | |
Barrel 3 zone temperature | 180 to 205 | °C | |
Barrel 5 zone temperature | 180 to 210 | °C | |
Melt temperature | 190 to 205 | °C | |
Nozzle temperature | 185 to 210 | °C |
Notes |
---|
1. Typical properties: these are not to be construed as specifications. |
2. Die C |
3. Post-cured 16 hr at 230°F |
4. Rate A (50°C/h), Loading 1 (10 N) |
【 Disclaimer 】 Guangzhou Soliao Information Technology Co., Ltd. reserves all rights. The information in this data table was obtained from the manufacturer of the material on soliao.com. Soliao.com makes every effort to ensure the accuracy of this data. However, the search company does not assume any responsibility for the uncertainty and consequences caused to users by these data values and suggestions, and strongly recommends verifying the data values with the material supplier before the final selection of materials. |