VALOX™ CS860 resin

About
30% 玻纤增强PBT+PET 共混物。颜色稳定。阻燃。家电用具:烫斗边缘、烤箱外表/面板

Product Description
SupplierSABIC
GenericPBT+PET
Material StatusCommercial: Active
FeaturesFlame Characteristics,Good color stability

Technical Data
MECHANICALNominal valueUnitTest method
tensile strength
Yield, Type I, 5 mm/min108MPaASTM D638
Fracture, Type I, 5 mm/min110MPaASTM D638
Tensile strain
Type I, 5 mm/min3.1%ASTM D638
Tensile modulus
5 mm/min6200MPaASTM D638
bending strength
Fracture, 50 mm span155MPaASTM D790
Bending modulus
8270MPaASTM D790

IMPACTNominal valueUnitTest method
Impact strength of cantilever beam at 23 ℃
No gap534J/mASTM D 4812
Gap80J/mASTM D 256

THERMALNominal valueUnitTest method
Hot deformation temperature
Unannealed, 6.4 mm
Relative temperature index
0.45 MPa212ASTM D 648
Electrical performance130UL 746B
1.8MPa187ASTM D 648
Impact mechanical performance130UL 746B
Non mechanical impact performance140UL 746B

PHYSICALNominal valueUnitTest method
Density1.73g/cm³ASTM D792
Shrinkage rate
3.2 mm
Melt Flow Rate
266℃,5.0kg45g/10minASTM D1238
MD0.2-0.3%SABIC Method
TD0.5-0.6%SABIC Method

Electrical performanceNominal valueUnitTest method
Arc resistance
Tungsten wire5PLC CodeASTM D495
Hot wire ignition {PLC}0PLC CodeUL 746A
High voltage arc marking rate {PLC}4PLC CodeUL 746A
High current arc ignition (surface {PLC})0PLC CodeUL 746A
Compared to the leakage tracing index3PLC CodeUL 746A

FLAME CHARACTERISTICSNominal valueUnitTest method
Flame retardant level
0.76 mmV-0UL 94
2.99 mm5VAUL 94

Process Conditions
Injection moldingNominal valueUnitTest method
Drying temperature60 – 75°C
Drying time4 – 5hrs
Drying time (gradually increasing)8hrs
Maximum water content0.05%
Minimum moisture content0.02%
Melt temperature255 – 275°C
Nozzle temperature255 – 270°C
Front temperature255 – 265°C
Mid section temperature250 – 260°C
Post stage temperature245 – 255°C
Mold temperature65 – 95°C
Back pressure0.3 – 0.7MPa
Screw speed50 – 80rpm
Shooting cylinder size40 – 80%
Depth of exhaust groove0.025 – 0.038mm

Notes
【 Disclaimer 】
Guangzhou Soliao Information Technology Co., Ltd. reserves all rights. The information in this data table was obtained from the manufacturer of the material on soliao.com. Soliao.com makes every effort to ensure the accuracy of this data. However, the search company does not assume any responsibility for the uncertainty and consequences caused to users by these data values and suggestions, and strongly recommends verifying the data values with the material supplier before the final selection of materials.