About |
---|
Standard flow, transparent, high purity polycarbonate copolymer resin with reduced oxygen permeability and water vapor transmission rate. For medical devices and pharmaceutical applications. Healthcare management of change, biocompatible (ISO 10993 or USP Class VI), food contact compliant.&& |
Product Description | |
---|---|
Supplier | SABIC |
Generic | Polycarbonate |
Material Status | Commercial: Active |
Features | High purity,Biocompatible,Food contact compliance,Poor moisture permeability,Copolymer |
Availabilitys | North America |
Process Methods | Injection Molding |
Technical Data | |||
---|---|---|---|
PHYSICAL | Nominal value | Unit | Test method |
Density | |||
— | 1.20 | g/cm³ | ASTM D792 |
— | 1.17 | g/cm³ | ISO 1183,ASTM D792 |
Specific volume | 0.850 | cm³/g | ASTM D792 |
Melt Flow Rate | |||
300℃,1.20kg | 15 | g/10min | ASTM D1238 |
Melt Volume Rate | |||
300℃,1.2 kg | 13.0 | cm³/10min | ISO 1133 |
Shrinkage rate | |||
MD:3.2 mm | 0.50 to 0.80 | % | Internal Method |
Water absorption rate | |||
24hr | 0.080 | % | ASTM D570 |
24hr,50% RH | 0.040 | % | ASTM D570 |
Saturation, 23 ℃ | 0.27 | % | ISO 62 |
Equilibrium, 23 ℃ | 0.28 | % | ASTM D570 |
Balance, 50% RH | 0.13 | % | ASTM D570 |
Equilibrium, 23 ℃, 50% RH | 0.13 | % | ISO 62 |
IMPACT | Nominal value | Unit | Test method |
---|---|---|---|
Charpy Notched Impact Strength | ISO 179/1eA | ||
-30℃ | 3.0 | kJ/m² | |
23℃ | 3.0 | kJ/m² | |
Charpy Unnotch Impact strength | ISO 179/1eU | ||
-30℃ | 47 | kJ/m² | |
23℃ | 无断裂 | ||
Impact strength of cantilever beam notch | |||
-30℃ | 30 | J/m | ASTM D256 |
23℃ | 30 | J/m | ASTM D256 |
-30℃ | 4.0 | kJ/m² | ISO 180-1A |
23℃ | 5.0 | kJ/m² | ISO 180-1A |
Notched impact strength of cantilever beam | |||
23℃ | 无断裂 | ASTM D4812, ISO 180/1U | |
-30℃ | 45 | kJ/m² | ISO 180/1U |
Dart impact equipped with measuring instruments | |||
23℃,Total Energy | 30.0 | J | ASTM D3763 |
THERMAL | Nominal value | Unit | Test method |
---|---|---|---|
Hot deformation temperature | |||
0.45 MPa, unannealed, 3.2 mm | 133 | ℃ | ASTM D648 |
0.45 MPa, unannealed, 100 mm span | 131 | ℃ | ISO 75-2/Be |
1.8 MPa, unannealed, 3.2 mm | 119 | ℃ | ASTM D648 |
1.8 MPa, unannealed, 100 mm span | 118 | ℃ | ISO 75-2/Ae |
Vicat Softening Temp | |||
— | 139 | ℃ | ASTM D1525 18 |
B50 | 138 | ℃ | ISO 306 |
B120 | 140 | ℃ | ISO 306/B120 |
Ball pressure test | IEC 60695-10-2 | ||
125℃ | Pass | ||
140℃ | Pass | ||
Linear coefficient of thermal expansion | |||
MD:-40~95℃ | 7.0E-5 | 1/℃ | ASTM E831 |
MD:23~80℃ | 7.0E-5 | 1/℃ | ISO 11359-2 |
TD:-40~95℃ | 7.0E-5 | 1/℃ | ASTM E831 |
TD:23~80℃ | 7.0E-5 | 1/℃ | ISO 11359-2 |
specific heat | 1400 | J/kg/℃ | ASTM C351 |
Thermal conductivity coefficient | 0.20 | W/m/K | ASTM C177, ISO 8302 |
Electrical performance | Nominal value | Unit | Test method |
---|---|---|---|
Volume resistivity | > 1.0E+17 | ohms·cm | ASTM D257 |
Dielectric constant | ASTM D150 | ||
50 Hz | 2.90 | ||
60 Hz | 2.90 | ||
1 MHz | 2.80 | ||
Compared to the leakage tracing index | PLC 2 | UL 746 |
optical performance | Nominal value | Unit | Test method |
---|---|---|---|
Refractive index | 1.584 | ASTM D542,ISO 489 | |
Transmittance | |||
2540 µm | 88.0 | % | ASTM D1003 |
Haze | |||
2540 µm | < 0.80 | % | ASTM D1003 |
MECHANICAL | Nominal value | Unit | Test method |
---|---|---|---|
Rockwell hardness | ASTM D785 | ||
Level L | 108 | ||
M-level | 93 | ||
Ball hardness | |||
H358/30 | 128 | MPa | ISO 2039-1 |
Erichson Scratch Depth(6N) | 14.0 | µm | Internal Method |
Pencil hardness | H | ASTM D3363 | |
Tensile modulus | |||
— | 2900 | MPa | ASTM D638 |
— | 2450 | MPa | ISO 527-1-2 |
tensile strength | |||
yield | 80.0 | MPa | ASTM D638 |
yield | 80.0 | MPa | ISO 527-2/50 |
fracture | 65.0 | MPa | ASTM D638 |
fracture | 60.0 | MPa | ISO 527-2/50 |
Tensile strain | |||
yield | 7.0 | % | ASTM D638 |
yield | 7.0 | % | ISO 527-2/50 |
fracture | 70 | % | ASTM D638 |
fracture | 40 | % | ISO 527-2/50 |
Bending modulus | |||
50 mm span | 2600 | MPa | ASTM D790 |
— | 2450 | MPa | ISO 178 |
bending strength | |||
— | 108 | MPa | ISO 178 |
Yield, 50 mm span | 120 | MPa | ASTM D790 |
Taber abraser | |||
1000 cycles, 1000 g, CS-17 wheels | 10.0 | mg | ASTM D1044 |
1000 cycles, 1000 g, CS-17 wheels | 10.0 | mg | Internal Method |
Process Conditions | |||
---|---|---|---|
injection | Nominal value | Unit | Test method |
Drying temperature | 120 | °C | |
Drying time | 3.0 to 4.0 | hr | |
Recommended maximum moisture content | 0.020 | % | |
Hopper temperature | 60.0 to 80.0 | °C | |
Barrel rear temperature | 260 to 280 | °C | |
Barrel middle temperature | 280 to 305 | °C | |
Barrel front temperature | 295 to 315 | °C | |
Nozzle temperature | 290 to 310 | °C | |
Processing (melt) temperature | 295 to 315 | °C | |
Mold temperature | 70.0 to 95.0 | °C |
Notes |
---|
【 Disclaimer 】 Guangzhou Soliao Information Technology Co., Ltd. reserves all rights. The information in this data table was obtained from the manufacturer of the material on soliao.com. Soliao.com makes every effort to ensure the accuracy of this data. However, the search company does not assume any responsibility for the uncertainty and consequences caused to users by these data values and suggestions, and strongly recommends verifying the data values with the material supplier before the final selection of materials. |