XENOY™ XL1339 resin

About
Data generated in BOZ labs. High heat grade for nonchemical resistance required applications.&&

Product Description
SupplierSABIC
GenericPC+PET
Material StatusCommercial: Active
FeaturesHigh Heat Resistance
AvailabilitysNorth America
Process MethodsInjection Molding

Technical Data
PHYSICALNominal valueUnitTest method
Density1.22g/cm³ASTM D792
Melt Volume Rate
265℃,1.2 kg4.00cm³/10minISO 1133
Shrinkage rate
TD0.50 to 0.80%Internal Method
MD0.50 to 0.80%Internal Method
Water absorption rate ASTM D570
24hr0.10%ASTM D570
Equilibrium, 23 ℃0.70%ASTM D570
Balance, 50% RH0.20%ASTM D570

MECHANICALNominal valueUnitTest method
Tensile modulus2100MPaASTM D638
tensile strength
fracture50.0MPaASTM D638
fracture40.0MPaISO 527-2/50
yield55.0MPaISO 527-2/50
yield50.0MPaASTM D638
Tensile strain
fracture110%ASTM D638
fracture70%ISO 527-2/50
yield5.0%ASTM D638
yield5.0%ISO 527-2/50
Bending modulus2200MPaISO 178
50 mm span2100MPaASTM D790
bending strength80.0MPaISO 178
bending strength
Yield, 50 mm span94.5MPaASTM D790
Poisson’s ratio0.40 ASTM D638
Taber abraser
1000 cycles, 1000 g, CS-17 wheels16.0mgASTM D1044

IMPACTNominal valueUnitTest method
Charpy Notched Impact Strength ISO 179/1eA
-30℃35kJ/m²ISO 179/1eA
23℃45kJ/m²ISO 179/1eA
Charpy Unnotch Impact strength ISO 179/1eU
-30℃No Break ISO 179/1eU
23℃No Break ISO 179/1eU
Impact strength of cantilever beam notch ASTM D256
-40℃220J/mASTM D256
-30℃250J/mASTM D256
-20℃600J/mASTM D256
0℃670J/mASTM D256
23℃700J/mASTM D256
Impact strength of cantilever beam notch ISO 180/1A
-40℃15kJ/m²ISO 180-1A
-30℃25kJ/m²ISO 180-1A
-20℃35kJ/m²ISO 180-1A
-10℃38kJ/m²ISO 180-1A
23℃40kJ/m²ISO 180-1A
Notched impact strength of cantilever beam ISO 180/1U
-30℃No Break ISO 180/1U
23℃No Break ISO 180/1U

THERMALNominal valueUnitTest method
Hot deformation temperature
1.8 MPa, unannealed, 100 mm span105ISO 75-2/Ae
0.45 MPa, unannealed, 100 mm span125ISO 75-2/Be
Vicat Softening Temp 
A50140ISO 306/A50
B50130ISO 306
B120135ISO 306/B120
Linear coefficient of thermal expansion
TD:-30~30℃7.9E-51/℃ASTM D696
MD:-30~30℃7.6E-51/℃ASTM D696
Thermal conductivity coefficient0.18W/m/KASTM C177

Electrical performanceNominal valueUnitTest method
Surface resistivity> 1.0E+15ohmsASTM D257
Volume resistivity> 1.0E+14ohms·cmASTM D257
Dielectric strength
3.2 mm in oil17kV/mmASTM D149
Dielectric constant ASTM D150
50 Hz3.30 ASTM D150
60 Hz3.30 ASTM D150
1 MHz3.10 ASTM D150
Dissipation factor ASTM D150
50 Hz2.0E-3 ASTM D150
60 Hz2.0E-3 ASTM D150
1 MHz0.020 ASTM D150

Process Conditions
injectionNominal valueUnitTest method
Drying temperature110°C
Drying time4.0 to 6.0hr
Drying time, maximum8.0hr
Recommended maximum moisture content0.020%
Recommended injection volume50 to 80%
Barrel rear temperature243 to 266°C
Barrel middle temperature249 to 271°C
Barrel front temperature254 to 277°C
Nozzle temperature254 to 271°C
Processing (melt) temperature260 to 277°C
Mold temperature66 to 88°C
Back pressure0.345 to 0.689MPa
Screw speed50 to 80rpm
Vent depth0.013 to 0.020mm

Notes
1. Typical properties: these are not to be construed as specifications.
2. Tensile Bar
3. 2.0 in/min
4. Type I, 2.0 in/min
5. 0.051 in/min
6. 0.079 in/min
7. Yield
8. 80*10*4 sp=62mm
9. 80*10*4
10. 120*10*4 mm
【 Disclaimer 】
Guangzhou Soliao Information Technology Co., Ltd. reserves all rights. The information in this data table was obtained from the manufacturer of the material on soliao.com. Soliao.com makes every effort to ensure the accuracy of this data. However, the search company does not assume any responsibility for the uncertainty and consequences caused to users by these data values and suggestions, and strongly recommends verifying the data values with the material supplier before the final selection of materials.